In this study, wear prosess was carried out with graphide electrode in EDM at different processing parameters of AISI 1.2738 material. The parameters used in the experimental study were determined after the preliminary experiments. This parameters were determined as three different pulse durations (100, 200 and 300 µs), waitingperiod (10, 20 and 30 µs) and discharge current (10, 20 ve 30 amper). As a result of the analysis, it was found out that the lowest average surface roughness value were 100 µs pulse durations, 10 µs waiting-period and 20 amper discharge current and on the other hand, the highest average surface roughness values were found 300 µs pulse durations, 10 µs waiting-period and 30 amper discharge current.
Bu çalışmada, AISI 1.2738 malzemenin farklı işleme
parametrelerinde elektro erozyon tezgahında grafit elektrot ile aşındırma
işlemi gerçekleştirilmiştir. Deneysel çalışmada kullanılan parametreler yapılan
ön deneyler sonrasında üç farklı vurum süresi (100, 200 ve 300 µs), bekleme
süresi (10, 20 ve 30 µs) ve boşalım akım
(10, 20 ve 30 amper) olarak belirlenmiştir. Yapılan çalışmanın sonucunda
en düşük yüzey pürüzlülük değerinin 100 µs vurum süresi, 10 µs bekleme süresi
ve 20 amper akımda gerçekleştiği, en yüksek yüzey pürüzlülük değerinin ise 300
µs vurum süresi, 10 µs bekleme süresi ve 30 amper akımda gerçekleştiği
belirlenmiştir.
Birincil Dil | Türkçe |
---|---|
Konular | Mühendislik |
Bölüm | Makaleler |
Yazarlar | |
Yayımlanma Tarihi | 10 Nisan 2018 |
Yayımlandığı Sayı | Yıl 2018 Cilt:6 Sayı:3 (2018) (Özel Sayı: UMAS 2017) |