In this study, flotation tests on samples obtained from Tunçbilek Coal Preparation Plant were done
firstly, using an oily collector and frother. Afterwards, block co-polymers were used in addition to
collector and frother to improve floatability of coal selectively. Three different polymers, pluronic L-64,
P-104 and 10R-8, were tested in lignite flotation in this study. At the end of the study, lignite was
floated with 67,19% combustible matter recoveries and 17,65% ash content in 4 minutes flotation
without polymers. 73,25% combustible matter recoveries were obtained with'L-64 polymer addition;
while it is determined that flotation recoveries were not improved with P-104 polymer addition. Although
about 80% combustible matter recovery values were attained with 10R-8 polymer, ash contents of
clean coal products were also increased.
Bu çalışmada, Tunçbilek Lavvan'ndan alınan numuneler üzerinde öncelikle toplayıcı ve köpürtücü
kullanarak flotasyon deneyleri yapılmıştır. Sonrasında kömürün sellektif yüzdürülebilirliğinin arttırılması
amacıyla toplayıcı ve köpürtücüye ilave olarak blok ko-polimerler kullanılmıştır. Çalışmada pluronik L-
64, P-104 ve 10R-8 olmak üzere üç tip polimer linyit flotasyonunda denenmiştir. Sonuç olarak linyitin
polimersiz olarak 4 dakika flotasyon sonucunda %67,19 yanıcı madde ve %17,65 kül oranı ile
yüzdürülebildiği tespit edilmiştir. L-64 polimerinin ilavesi ile yapılan deneylerde %73,25 yanıcı madde
verimi değerleri elde edilirken, P-104 polimerinin flotasyon verimine bir katkısı olmadığı belirlenmiştir.
10R-8 polimeri ile yaklaşık olarak %80 yanıcı madde verimi değerlerine ulaşılmış olmasına rağmen
paralelinde konsantrenin kül oranında da artış gerçekleşmiştir.
Linyit Flotasyonu Blok Ko-Polimerler İnce Kömürün Zenginleştirilmesi
Diğer ID | JA38AR42JP |
---|---|
Bölüm | Araştırma Makalesi |
Yazarlar | |
Yayımlanma Tarihi | 1 Mart 2004 |
Gönderilme Tarihi | 1 Mart 2004 |
Yayımlandığı Sayı | Yıl 2004 Cilt: 43 Sayı: 1 |