Dissolution of Ulexite in Hydrochloric Acid Solutions
Abstract
Ulexite is an important boron mineral used for the
production of boron compounds. Purpose of the study has been to investigate the
dissolution of ulexite in hydrochloric acid solutions in a batch reactor and to
present an alternative process to produce boric acid. Reaction temperature,
particle size, solid/liquid ratio, acid concentration and stirring speed have
been selected as parameters on the dissolution rate of ulexite. The parameters
used in experiments are; acid concentration 0.75*,1,1.25,1.5,2M,
reaction temperature 30*,40,50,60,70oC, particle size
-14+18*,-18+30,-30+40,-40+50,-50+60 mesh, solid/liquid ratio
5/100,7.5/100,10/100* g/mL, stirring speed 500*,650,800
rpm. It has been found that the dissolution rate has increased the reaction
temperature and the stirring speed. However, increasing the particle size, acid
concentration and solid/liquid ratio have decreased the rate of dissolution.
Keywords
Kaynakça
- Abali Y, Bayca S.U, Mistincik, E, (2006). Kinetics of oxalic acid leaching of tincal. Chemical Engineering Journal.
- (123): 25–30.
- Demirkıran N, Künkül A, (2007). Dissolution kinetics of ulexite in perchloric acid solutions. Int. J. Miner. Process.
- (83):76–80.
- Doğan T, Yartaşı A, (2009). Kinetic investigation of reaction between ulexite ore and phosphoric acid. Hydrometallurgy.
- 294-299.
- Durak H., Genel Y.,(2012). Analysis of leaching kinetics of tincal in phosphoric acid solutions in high temperatures.
- Scientific Research and Essays Vol. 7(40), pp. 3428 3441.
Ayrıntılar
Birincil Dil
İngilizce
Konular
-
Bölüm
Araştırma Makalesi
Yayımlanma Tarihi
31 Aralık 2016
Gönderilme Tarihi
1 Ocak 2017
Kabul Tarihi
25 Aralık 2016
Yayımlandığı Sayı
Yıl 2016 Cilt: 1 Sayı: 1